Vohringer Gmbh Laminate Wood Flooring Germany
Vohringer laminate flooring are put through stringent tests for strength, durability and moisture resistance to ensure that they comply with European and International Standards. And in order to ensure the rigour of daily use over a long period of time, all of them surpass these standards.
Testing of Vohringer laminate wood floor according to DIN EN 13329 | ||
TYPE | TEST STANDARD | RESULT |
Abrasion Resistance | AC5 IP ≥ 6500 AC4 IP ≥ 4000 |
6600 revolutions 4200 revolutions |
Impact Resistance | IC3 IC2 |
IC3 IC2 |
Resistance to Staining | 5, groups 1 and 2 4, group 3 |
5, groups 1 and 2 4, group 3 |
Resistance to cigarette burns | ≥ Grade 4 | Grade 5 |
Effect of a furniture leg | EN 424 | No visible damage |
Effect of a castor leg | EN 425 | No visible damage |
Thickness Swelling | ≤ 18 % | ≤ 8 % |
Squareness of the element , q | q max ≤ 0,20 mm | q max = 0,20 mm |
Straightness of the surface layer, s | s max ≤ 0,30 mm/m | s max = 0,15 mm/m |
Dimensional variations after changes in relative humidity, δ1,δw | δ1 average ≤ 0,9 mm δw average ≤ 0,9 mm |
δ1 average = 0,6 mm δw average = 0,8 mm |
Light fastness | Blue wool scale, not worse than 6 Grey scale, not worse than 4 |
Blue wool scale: > 6 Grey scale: > 4 |
Static Indentation | No visible change, i.e. ≤0,01 mm indentation using a straight steel cylander, ø = 11,30 mm | No visible change, 0,00 mm indentation |
Surface Soundness | ≥1,00 N/mm2 | 1,47 N/mm2 |
Other Technical Data of Vohringer Laminate Wood Flooring: | ||
TYPE | TEST STANDARD | RESULT |
Formaldehyde emission | EN 717 | E1 |
Behavior in fire | DIN 4102 | Low flammability, building class B1 |
Reaction to fire | GB/T 18102-2000 | No visible changes |
Flammability classification | VKF-Schweiz | Fire protection classification 5.3 |
Overlay bond | > 1,0 MPa | 2,31 MPa |
Internal bond | > 1,0 MPa | 1,19 MPa |
Slip Resistance | EN 13893 | Pass |